| All data is for information only------(<---links) | |
|---|---|
| PRODUCT DATA of Grade 1 | 
| Material | Grade 1 | 
| Product Datasheet | Grade 1 | 
| Precautions | Strong affinity for hydrogen (above 130 C), nitrogen (above 800 C) and oxygen above 700 C which cause embrittlement. | 
| Chemical Composition | 99.5 Ti | 
| EXPERIENCE IN PRACTICE | 
|---|
| Equivalent Designations | ASTM Grade 1, UNS R50250, CP titanium | 
| PHYSICAL PROPERTIES | 
|---|
| Specific Gravity | 4.51 | 
| Phase changes | Beta transus 888 C | 
| ELASTIC PROPERTIES | 
|---|
| Tensile Modulus | 105 GPa | 
| Shear Modulus | 45 GPa | 
| Poisson Ratio | 0.37 | 
| ELECTRICAL PROPERTIES | 
|---|
| Electrical Volume Resistivity | 4.5e-7 ohm.m | 
| THERMAL PROPERTIES | 
|---|
| Thermal Conductivity | 16 W/m.K | 
| Thermal Expansion Coefficient | 8.6 μstrain/°C | 
| Melting Range | 1670 °C(maximum) | 
| Specific Heat | 0.52 J/g.K | 
| SPECIAL RECOMMENDATIONS | 
|---|
| Lessons Learned | Welding procedures should always be checked. Argon or helium protection is essential on trailing direction and opposite side. |