All data is for information only------(Home) | |
---|---|
PRODUCT DATA of Grade 2 |
Material | Grade 2 |
Product Datasheet | Ti grade 2 |
Precautions | Strong affinity for hydrogen (above 130 C), nitrogen (above 800 C) and oxygen above 700 C which cause embrittlement |
Chemical Composition | 99.2 Ti |
EXPERIENCE IN PRACTICE |
---|
Equivalent Designations | ASTM Grade 2; UNS R50400, CP titanium |
PHYSICAL PROPERTIES |
---|
Specific Gravity | 4.51 |
Phase changes | Beta transus 913 C |
ELASTIC PROPERTIES |
---|
Tensile Modulus | 105 GPa |
Shear Modulus | 45 GPa |
Poisson Ratio | 0.37 |
MECHANICAL PROPERTIES |
---|
Ultimate Tensile Strength | 344 MPa |
Proof Stress (0.2%) | 275 to 410 MPa |
Elongation | 20 % |
Reduction in Area | 35 % |
Fatigue Limit | 300 MPa Remark:Unnotched 10^7 cycles |
Fracture Toughness (KIc) | Remark:K(q), annealed |
ELECTRICAL PROPERTIES |
---|
Electrical Volume Resistivity | 4.5e-7 ohm.m |
THERMAL PROPERTIES |
---|
Thermal Conductivity | 16.4 W/m.K |
Thermal Expansion Coefficient | 8.6 μstrain/°C |
Specific Heat | 0.523 J/g.K |
Melting Range | 1670 °C(maximum) |
SPECIAL RECOMMENDATIONS |
---|
Lessons Learned | Welding procedures should always be checked. Argon or helium protection is essential on trailing direction and opposite side. |