| Data still to be completed------(Home) | |
|---|---|
| PRODUCT DATA of CDA 782 |
| Material | CDA 782 |
| General Information | Typical data from standards handbook of copper and copper alloys (Copper.org) @ Room Temperature |
| Chemical Composition | Cu-8Ni-2Pb-25Zn |
| EXPERIENCE IN PRACTICE |
|---|
| Equivalent Designations | CDA782 |
| PHYSICAL PROPERTIES |
|---|
| Specific Gravity | 8.69 |
| ELASTIC PROPERTIES |
|---|
| Tensile Modulus | 117 GPa |
| Shear Modulus | 44.1 GPa |
| ELECTRICAL PROPERTIES |
|---|
| Electrical Volume Resistivity | 1.71e-7 ohm.m |
| THERMAL PROPERTIES |
|---|
| Thermal Conductivity | 48.5 W/m.K |
| Thermal Expansion Coefficient | 18.5 µstrain/°C |
| Specific Heat | 0.377 J/g.K |
| Melting Range | 971 to 999 °C |
| RELEVANT PROPERTIES FOR USE IN SPACE COMMUNITY |
|---|
| Stress Corrosion Status | Low Resistance to SCC: Table 3
Remark: in the 50% cold rolled condition only Remark: Requires Stress corrosion evaluation form Remark: acc. to ECSS-Q-ST-70-36C Data Quality: Design Data |