| Data still to be completed------(Home) | |
|---|---|
| PRODUCT DATA of CDA 524 |
| Material | CDA 524 |
| General Information | Typical data from standards handbook of copper and copper alloys (CDA inc) @ Room Temperature |
| Chemical Composition | Cu-10Sn-0.3P |
| EXPERIENCE IN PRACTICE |
|---|
| Equivalent Designations | C52400; CuSn10; CuSn10P; C-7160; CDA524; Phosphor Bronze, 10% |
| PHYSICAL PROPERTIES |
|---|
| Specific Gravity | 8.78 |
| ELASTIC PROPERTIES |
|---|
| Tensile Modulus | 110 GPa |
| Shear Modulus | 41.2 GPa |
| ELECTRICAL PROPERTIES |
|---|
| Electrical Volume Resistivity | 1.57e-7 ohm.m |
| THERMAL PROPERTIES |
|---|
| Thermal Conductivity | 50.2 W/m.K |
| Thermal Expansion Coefficient | 18.4 µstrain/°C |
| Specific Heat | 0.377 J/g.K |
| Melting Range | 845 to 1000 °C |
| RELEVANT PROPERTIES FOR USE IN SPACE COMMUNITY |
|---|
| Stress Corrosion Status | High Resistance to SCC: Table 1
Remark: in the 0% cold rolled condition only Remark: acc. to ECSS-Q-ST-70-36C Data Quality: Design Data |