Data still to be completed------(Home) | |
---|---|
PRODUCT DATA of CDA 762 |
Material | CDA 762 |
General Information | Typical data from standards handbook of copper and copper alloys (Copper.org) @ Room Temperature |
Chemical Composition | Cu-28.5Zn-12.2Ni |
EXPERIENCE IN PRACTICE |
---|
Equivalent Designations | C76200; CuNi12Zn29; CW405J; CDA762 |
PHYSICAL PROPERTIES |
---|
Specific Gravity | 8.58 |
ELASTIC PROPERTIES |
---|
Tensile Modulus | 124 GPa |
Shear Modulus | 46.9 GPa |
ELECTRICAL PROPERTIES |
---|
Electrical Volume Resistivity | 1.92e-7 ohm.m |
THERMAL PROPERTIES |
---|
Thermal Conductivity | 45 W/m.K |
Thermal Expansion Coefficient | 16.2 µstrain/°C |
Specific Heat | 0.377 J/g.K |
Melting Range | 980 to 1020 °C |
RELEVANT PROPERTIES FOR USE IN SPACE COMMUNITY |
---|
Stress Corrosion Status | Low Resistance to SCC: Table 3
Remark: in the annealed, 25% or 50% cold rolled condition only Remark: Requires Stress corrosion evaluation form Remark: acc. to ECSS-Q-ST-70-36C Data Quality: Design Data |