| All data is for information only------(Home) | |
|---|---|
| PRODUCT DATA of AA7079-T6 |
| Material | AA7079-T6 |
| General Information | Obsolete Alloy |
| Processing and Assembly | Solution heat treated and artificially aged |
| Precautions | Typical data from AA |
| EXPERIENCE IN PRACTICE |
|---|
| Development Status | Commercial Product |
| Equivalent Designations | AA 7079 |
| PHYSICAL PROPERTIES |
|---|
| Specific Gravity | 2.76 |
| Magnetic Properties | Nonmagnetic |
| ELASTIC PROPERTIES |
|---|
| Tensile Modulus | 72 GPa |
| MECHANICAL PROPERTIES |
|---|
| Ultimate Tensile Strength | 538 MPa |
| Proof Stress (0.2%) | 469 MPa |
| Elongation | 14 % |
| Fatigue Limit | 159 MPa |
| Hardness | 145 HB |
| Shear Strength | 310 MPa |
| RELEVANT PROPERTIES FOR USE IN SPACE COMMUNITY |
|---|
| General Corrosion Status | Requires specific corrosion protection |
| Stress Corrosion Status | Low Resistance to SCC: Table 3 Data Quality: Design Data |