| Data still to be completed------(<---links) | |
|---|---|
| PRODUCT DATA of CDA 917 |
| Material | CDA 917 |
| General Information | cast alloy Data @ Room Temperature |
| Chemical Composition | Cu-12Sn-2Ni |
| EXPERIENCE IN PRACTICE |
|---|
| Equivalent Designations | C91700; CuSn12Ni2-B; CB484K; CuSn12NI; 2.1060; CT2; CDA917 |
| PHYSICAL PROPERTIES |
|---|
| Specific Gravity | 8.75 |
| ELASTIC PROPERTIES |
|---|
| Tensile Modulus | 103 GPa |
| ELECTRICAL PROPERTIES |
|---|
| Electrical Volume Resistivity | 1.72e-7 ohm.m |
| THERMAL PROPERTIES |
|---|
| Thermal Conductivity | 70.6 W/m.K |
| Thermal Expansion Coefficient | 16.2 µstrain/°C |
| Melting Range | 851 to 1010 °C |
| Specific Heat | 0.377 J/g.K |
| RELEVANT PROPERTIES FOR USE IN SPACE COMMUNITY |
|---|
| Stress Corrosion Status | High Resistance to SCC: Table 1
Remark: in the 0% cold rolled condition only Remark: acc. to ECSS-Q-ST-70-36C Data Quality: Design Data |